shoe materials

Shoe Materials

Recipe Application:

product

Shoe material

How to use

Results

type

part

Activated rubber powder C

Sporty and comfortable

Rubber outsole

Partial replacement

NR/BR/white carbon black

.Hardness and physical properties: consistent with the original formula

. Wear: Same as the original formula performance


Application of shoe material rubber outsole formula: two yuan becomes three yuan

Principle of adjusting the main ingredients of the formula:


Application of shoe material rubber outsole formula: formula adjustment, cost reduction and efficiency improvement

Note: Adjust the usage of NR and activated rubber powder C based on the original XL formula.

plan

XL

A1

Purpose

Original recipe

Cost savings

Cost saving Yuan/ton (quality cost)

0

-480

NR

80

-5

BR9000

20


White Carbon Black

55


Activated rubber powder C

0

+10

Reduce the amount of NR: the purpose is to reduce costs  


Customer test application feedback: rubber outsole (non-foamed)

plan

XL

A1

Purpose

Original recipe

Cost savings

Cost saving Yuan/ton (quality cost)

0

-480

NR

80

-5

BR9000

20


White Carbon Black

55


Activated rubber powder C

0

10

Curing conditions: 165℃*8min

Appearance

Smooth, clean and spotless

Smooth, clean and spotless

proportion

1.135

1.134

hardness

61

62

Tensile strength TB/MPa

17

17.1

Elongation at break EB/%

478

455

Wear

0.34

0.33

Data analysis (activated rubber powder C: 10phr)

Hardness: The hardness is consistent with the original formula;

Physical properties: tensile strength is consistent with the original formula;

Abrasion: Excellent abrasion performance;

Appearance: smooth, clean and spotless.


in conclusion

Through the above formula experiments and customer usage verification, Star activated rubber powder can reduce costs and increase efficiency in the shoe material application market with significant results.

Welcome to use it and work together to further develop the application market!